Structural alloy steel 36HNM, 36CrNiMo4, 1.6511 for thermal improvement for heavy-duty parts of machines, motors and aircraft, according to PN-72/H-84030, PN-89/H-84030.04 and PN-EN 10083-1.

 

Standards Steel Grades
Chemical Composition %
C: Mn: Si: P: S: Cr: Mo: Ni:
PN 36HNM
0.32 - 0.40 0.50 - 0.80 0.17 - 0.37 <0.035 <0.035 0.90 - 1.20 0.15 - 0.25 0.90 - 1.20
EN 36CrNiMo4 - 1.6511 
0.32 - 0.40 0.50 - 0.80 <0.40 <0.035 <0.035 0.90 - 1.20 0.15 - 0.30 0.90 - 1.20
GOST 36ChNM - 36KhNM - 36ХНМ
0.32 - 0.40 0.50 - 0.80 <0.40 <0.035 <0.035 0.90 - 1.20 0.15 - 0.30 0.90 - 1.20
PN 34HNM
0.32 - 0.40 0.40 - 0.70 0.17 - 0.37 <0.035 <0.035 1.30 - 1.70 0.15 - 0.25 1.30 - 1.70
EN 34CrNiMo6 - 1.6582 - 34 CrNiMo 6
0.30 - 0.38 0.50 - 0.80 <0.40 <0.025 <0.035 1.30 - 1.70 0.15 - 0.30 1.30 - 1.70
AFNOR 35NCD2 - 35 NCD 2
0.32 - 0.40 0.70 - 1.00 0.10 - 0.40 <0.040 <0.035 0.40 - 0.60 0.15 - 0.30 0.40 - 0.70
ČSN
STN
ČSN 16343 - ČSN 16 343
0.32 - 0.40 0.50 - 0.80 0.15 - 0.40 <0.035 <0.035 1.30 - 1.70 0.20 - 0.30 1.30 - 1.70

 

Steel 36HNM - description and specification

Structural alloy steel with high hardness and toughness for thermal improvement characterized by high resistance to impact, twisting, and vibration. The best mechanical properties reach at dimensions of about 80mm after hardening in oil, and at 100mm after hardening in water.

In addition, it does not show sensitivity to the temper brittleness. Used for machine parts, motor vehicles, engine parts and aircrafts, heavy-duty components of road and mining machinery.

The 36HNM steel is used to made connecting rods, control parts, crushed shafts, press parts, shafts for motors, shafts of larger diameter steam turbines, control parts, heavy duty screws and screws, shipbuilding parts operating at temperatures up to 400 ℃ , single disc and quartz rotors, shafts for pumps, and drilling components in the oil industry.


Mechanical properties of 36HNM steel

Properties of 36HNM steel
Tensile strength Rm > 830 MPa
Yield point Re > 690 MPa
Notch toughness KU2 > 96 J
Elongation A > 15 %
Contraction Z > 55 %
Density ρ ~7,85 kg/dm3
Hardness in softened state HB < 217 HB

 

Properties Dimensions
<16mm 16 - 40mm 40 - 100mm 100 - 160mm 160 - 250mm
Tensile strength Rm 1080 - 1250 MPa 980 - 1130 MPa 880 - 1030 MPa 780 - 930 MPa 740 - 880 MPa
Yield point Re > 880 MPa > 780 MPa > 690 MPa > 590 MPa > 540 MPa
Notch toughness KU2 > 48 J > 64 J > 48 J > 48 J -
Contraction Z > 45 % > 50 % > 50 % > 55 % > 55 %
Elongation A > 10 % > 11 % > 12 % > 14 % > 14 %

 


Heat treatment of steel 36HNM, 36CrNiMo4, 1.6511

Heat treatment - processes
Process Cooling type Temperature
Normalizing annealing in calm air 850 - 880℃
Softening annealing slow 650 - 700℃
Hardening in oil 830 - 860℃
in water 820 - 840℃
Tempering in air 540 - 680℃

 


Welding, joining and cutting of 36HNM steel

36HNM grade is hard to weld steel grade. Products are welded under exceptional circumstances with arc or CO2 welding, preferably in a softened state. Before welding, the steel needs to be heated to the appropriate temperature depending on the dimensions of the product.

In the case of welding in the heat-treated state, the joining points and their periphery will lose some of the acquired properties, and then the best solution is to perform a suitable heat treatment. After the welding process, even before the product has cooled, the material at the joining points should be tempered or softened.

In cases where there are no conditions for heat treatment, the products should be cooled slowly with the furnace or in hot sand.

When cutting, the products must be heated to 250 - 350 ℃ and the cutting can be made with oxyacetylene blowpipe, propane-butane-oxygen torch or plasma torch. Cut products should be cooled in the air.

36HNM steel can also be joined - by electric welding, friction welding or resistance welding in a softened or heat-treated state. Welded products may exhibit slight differences, bearing in mind the properties of steel.

Temperatures of 36HNM products prior to welding
przekrój temperature
≤ 15mm 150 - 300℃
15 - 25mm 250 - 350℃
≥ 25mm 300 - 400℃

 


In the 36HNM grade the company provides:

 


List of other designations and equivalents of 36HNM steel:

36CrNiMo4, 1.6511, 36ChNM, 36KhNM, 36ХНМ, 34HNM, 35 NiCrMo 4, 35NiCrMo4, 35 NCD 4, 34CrNiMo6, 1.6582, 34 CrNiMo 6, 35NCD2, 35 NCD 2, ČSN 16343, ČSN 16 343.


We use cookies
In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy. You can specify the detailed configuration by clicking the button below "Settings".
Cookie settings
We use cookies

In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy.

More information

If you have any questions about our cookie policy, please ask contact.