Special structural alloy steel 32CDV13, 33CrMoV12-9, 32CrMoV12-9, 1.8522, AMS 6481 according to AIR 9160/C.

 

StandardsSteel Grades
Chemical Composition %
C:Mn:Si:P:S:Cr:Ni:Mo:V:Cu:
AIR 916032CDV13
0.29 - 0.360.4 - 0.70.1 - 0.4<0.025<0.0252.8 - 3.3<0.30.7 - 1.20.15 - 0.35-
EN32CrMoV12-9 - 33CrMoV12-9 - 1.8522
0.29 - 0.360.4 - 0.7<0.4<0.025<0.0352.8 - 3.3-0.7 - 1.00.15 - 0.25-
EN33CrMoV12
0.29 - 0.360.4 - 0.70.1 - 0.4<0.020<0.0202.8 - 3.8<0.30.7 - 1.20.15 - 0.35-
ASTMUNS K24340 - AMS 6481
0.29 - 0.360.4 - 0.70.1 - 0.4<0.015<0.0052.8 - 3.3<0.30.7 - 1.20.15 - 0.35<0.1

 

32CDV13, 32CrMoV12-9, 1.8522 - specification and applications

Structural steel with good hardening properties for nitriding used in the production of components requiring high impact resistance, fatigue, ductility and hardness in the aerospace and machinery industries.

The 32CrMoV12-9 grade is mainly used in the manufacture of heavy-duty machine parts such as rings, bearings, axles, crankshafts, flanges, aircraft parts, cogwheels, and gears. Correctly selected chemical composition allows the work of components to temperatures up to 400 ℃.


The mechanical properties of 32CrMoV12-9/33CrMoV12-9/1.8522 steel according to EN 10085

  • Delivery condition +A:
    • Hardness: < 248 HB
  • Delivery condition +QT - dimensions 16 - 40mm
    • Tensile strength, Rm: 1150 - 1350 MPa
    • Yield point, Rp0,2: >950 MPa
    • Elongation, A: >11%
    • Impact resistance, KV: >30J
  • Delivery condition +QT - dimensions 40 - 100mm
    • Tensile strength, Rm: 1050 - 1250 MPa
    • Yield point, Rp0,2: >850 MPa
    • Elongation, A: >12%
    • Impact resistance, KV: >35J
  • Delivery condition +QT - dimensions 100 - 160mm
    • Tensile strength, Rm: 950 - 1150 MPa
    • Yield point, Rp0,2: >750 MPa
    • Elongation, A: >12%
    • Impact resistance, KV: >40J
  • Delivery condition +QT - dimensions 160 - 250mm
    • Tensile strength, Rm: 900 - 1100 MPa
    • Yield point, Rp0,2: >700 MPa
    • Elongation, A: >13%
    • Impact resistance, KV: >45J

 


Thermal treatment of 32CrMoV12-9, 1.8522 - processes and temperatures:

  • Softening annealing is carried out at a temperature of 680 - 720℃
  • Hardening in oil or water at 870 - 970℃
  • Tempering at 580 - 700℃
  • Nitriding of surface is carried out in the range 480 - 570℃

 


In the above mentioned grades the company provides:

 


The other alternatives and substitutes:

32CDV13, 32CrMoV12-9, 33CrMoV12-9, 1.8522, UNS K24340, AMS 6481, 33CrMoV12, FE-PL1504, E32CDV13.


We use cookies
In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy. You can specify the detailed configuration by clicking the button below "Settings".
Cookie settings
We use cookies

In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy.

More information

If you have any questions about our cookie policy, please ask contact.