Structural boiler steel for nitriding 30CrMoV9, 1.7707, 31CrMoV9, 1.8519 according to DIN 17200, EN 10250-3, EN 10085.

 

Standard Steel Grade
Chemical Composition %
C: Mn: Si: P: S: Cr: Ni: Mo: V: Cu:
PN 33H3MF
0.29 - 0.36 0.5 - 0.8 0.17 - 0.37 <0.035 <0.035 2.4 - 2.8 <0.3 0.35 - 0.45 0.2 - 0.3 <0.3
PN 30H2MF
0.26 - 0.34 0.4 - 0.7 0.15 - 0.40 <0.035 <0.035 2.3 - 2.7 - 0.15 - 0.25 0.1 - 0.2 <0.3
EN 31CrMoV9 - 1.8519
0.27 - 0.34 0.4 - 0.7 <0.40 <0.025 <0.035 2.3 - 2.7 - 0.15 - 0.25 0.1 - 0.2 -
EN 30CrMoV9 - 1.7707
0.26 - 0.34 0.4 - 0.7 <0.40 <0.035 <0.035 2.3 - 2.7 <0.6 0.15 - 0.25 0.1 - 0.2 -
GOST 30Ch3MF - 30Х3МФ
0.27 - 0.34 0.3 - 0.6 0.17 - 0.37 <0.035 <0.035 2.3 - 2.7 <0.3 0.2 - 0.3 0.06 - 0.12 <0.3

 

31CrMoV9, 30CrMoV9, 1.7707, 1.8519 - specifications and application

30H2MF steel is boiler grade, low-alloyed, used in the energy industry for the parts working in high temperatures below 540 °C. The material is often used in the manufacture of screws, nuts, parts of turbines and other equipment for the energy industry.

33H3MF is a steel designed for nitriding, which, unlike 38HMJ, does not have Aluminum in its chemical composition. The grade can be interchangeably used, however, does not exhibit the same hardness after thermo-chemical treatment, as 38HMJ does. Steel intended for piston pins, gears, bushings, camshafts, engine components, valve parts, cylinders, etc.

Steel is not suitable for welding.


Mechanical properties of 31CrMoV9, 1.8519 +QT steel

  • Annealed softened delivery condition +A
    • Hardness, HB: <248
  • Heat-treated condition +QT
    • Tensile strength, Rm: 850 - 1300 MPa
    • The yield point, Re: > 650 MPa
    • Elongation, A:> 9%
    • Impact resistance, KV: > 25J
  • Hardness of surface after nitriding, HV1: 800

 


Mechanical properties of 30CrMoV9, 1.7707 +QT steel

  • Tensile strength, Rm: >800 MPa
  • The yield point, Rp0,2: >590 MPa
  • Elongation, A:> 8%
  • Impact resistance, KV: > 20J

 

Temperature (℃) 200 300 400
The yield point Rp0.2 >620 MPa >540 MPa >480 MPa

 


Mechanical properties of 33H3MF steel - 30mm section

  • Tensile strength, Rm: >1080 MPa
  • The yield point, Re: > 980 MPa
  • Elongation, A:> 13%
  • Contraction, Z: >57%
  • Impact resistance, KCU2: 118 J/cm3

 


Mechanical properties forgings 30H2MF - dimensions <100mm

  • Tensile strength, Rm: 1080 - 1270 MPa
  • The yield point, Re: > 880 MPa
  • Elongation, A:> 10%
  • Impact resistance, KV: > 20J

 

Temperature (℃) 200 300 400
The yield point Rp0.2 >706 MPa >603 MPa >539 MPa

 


In the above mentioned grades the company provides:

 


Other grades designations:

30 CrMoV 9, 31 CrMoV 9, 31CrMoV9, 30CrMoV9, 1.7707, 1.8519, 30Ch3MF, 30H2MF, 30Kh3MF, 30Х3МФ


We use cookies
In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy. You can specify the detailed configuration by clicking the button below "Settings".
Cookie settings
We use cookies

In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy.

More information

If you have any questions about our cookie policy, please ask contact.