Case-hardening steel 20Ch2N4A intended for heavy duty parts of aircrafts and aircraft structures according to PN-72/H-84035.

 

StandardsSteel Grades
Chemical composition %
C:Mn:Si:P:S:Cr:Mo:Ni:V:Ti:Cu:N:W:
PN20H2N4A
0.16 - 0.220.30 - 0.600.17 - 0.37<0.030<0.0251.25 - 1.65-3.25 - 3.65--<0.2--
GOST20Ch2N4A - 20Х2Н4А - 20Kh2N4A
0.16 - 0.220.30 - 0.600.17 - 0.37<0.025<0.0251.25 - 1.65<0.153.25 - 3.65<0.05<0.03<0.3<0.008<0.2
UNE18NiCrMo14 - 18 NiCrMo 14 - F-1556 - F1556
0.14 - 0.200.40 - 0.700.15 - 0.40<0.035<0.0351.30 - 1.600.15 - 0.253.25 - 3.75-----
ČSN
STN
ČSN 16 523 - ČSN 16523
0.12 - 0.190.30 - 0.600.17 - 0.37<0.035<0.0351.20 - 1.75-3.25 - 4.00-----
SAE
AISI
SAE 3316 - AISI E3316 - AISI E 3316
0.14 - 0.190.45 - 0.600.20 - 0.35<0.025<0.0251.40 - 1.75-3.25 - 3.75-----
GB/T20Cr2Ni4A - 43203
0.17 - 0.230.30 - 0.600.17 - 0.37<0.025<0.0251.25 - 1.65-3.25 - 3.65--<0.25--
JISSFVQ 3 - SFVQ3
<0.230.20 - 0.40<0.40<0.020<0.0201.50 - 2.000.40 - 0.602.75 - 3.90<0.03----

 

20H2N4A - Description and purpose

Steel for thermal improvement and carburization with high nickel content intended to particularly heavy duty machine parts and aircraft engines. It is characterized by very good hardenability, high core strength and high hardness. Steel for large dimensions parts such as sprockets, heavy duty screws, rocker arms, piston pins, shafts and bushings Products mode of 20H2N4A steel grade are not suitable for welding.


Mechanical and physical properties

  • Tensile strength Rm > 1270 MPa
  • Yield point Re >1080 MPa
  • Notch toughness KU2 > 64 J
  • Contraction Z > 45%
  • Elongation A > 9%
  • Hardness in softened state < 269 HB
  • Thermal conductivity λ = ~33,5 W ⋅ m-1 K-1
  • Pojemność cieplna cp = 490 J ⋅ kg-1 K-1
  • Density ρ = ~7,83 kg/dm3
  • Linear Expansion Factor α = ~11,1 ⋅ 10-6 K-1

 


Heat treatment

  • Normalising annealing at 860 - 880 °C
  • Softening annealing at 640 - 680℃
  • Carburization at 870 - 900℃
  • Carbonitriding at 850 - 880℃
  • Hardening I in oil at 845 - 875℃
  • Hardening II in oil at 760 - 800℃
  • Tempering after carburization in air or oil at 150 - 210℃
  • Cyanidizing at 840 - 860℃
  • Tempering, in order to avoid the fragility, in oil or water at a temperature of 500 - 650℃

 


In the 20H2N4A grade the company provides:

 


Related equivalents and determination of steel:

20Ch2N4A, 20Kh2N4A, 18NiCrMo14, 18 NiCrMo 14, F-1556, F1556, ČSN 16 523, ČSN 16523, SAE 3316, AISI E3316, AISI E 3316, 20Cr2Ni4A, 43203, 20Cr2Ni4, 17NiCrMo14, 18NiCrMo14-6, 1.3533, SFVQ 3, SFVQ3, 20Х2Н4А


We use cookies
In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy. You can specify the detailed configuration by clicking the button below "Settings".
Cookie settings
We use cookies

In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy.

More information

If you have any questions about our cookie policy, please ask contact.