Case-hardening steel 16NiCr4, 1.5714, 16NiCrS4, 1.5715 intended for gear wheels according to EN 10084.

 

Standards Steel Grade
Chemical composition %
C: Mn: Si: P: S: Cr: Mo: Ni: Cu:
EN/DIN 16NiCr4 - 1.5714 - 16 NiCr 4
0.13 - 0.19 0.70 - 1.00 <0.40 <0.025 <0.035 0.60 - 1.00 - 0.80 - 1.10 -
EN/DIN 16NiCrS4 - 16 NiCrS 4 - 1.5715
0.13 - 0.19 0.7 - 1.0 <0.4 <0.025 0.02 - 0.04 0.6 - 1.0 - 0.8 - 1.1 -
BS 637H17 - 637 H 17 - 637M17 - 637 M 17
0.14 - 0.20 0.60 - 0.90 0.10 - 0.35 <0.035 <0.04 0.60 - 1.00 - 0.85 - 1.25 -
GOST 18ChGN1 - 18KhGN1 - 18ХГН1
0.16 - 0.21 0.60 - 0.90 <0.40 <0.025 <0.035 0.90 - 1.20 - 1.20 - 1.50 -
GOST 19ChGN - 19KhGN - 19ХГН
0.16 - 0.21 0.70 - 1.00 0.17 - 0.37 <0.035 <0.035 0.80 - 1.10 <0.1 0.80 - 1.10 <0.3
PN 17HGN
0.15 - 0.21 1.00 - 1.30 0.17 - 0.37 <0.035 <0.035 0.80 - 1.10 - 0.60 - 0.90 -
PN 15HGN
0.13 - 0.20 0.70 - 1.00 0.17 - 0.37 <0.035 <0.035 0.80 - 1.10 - 1.30 - 1.60 -

 

16NiCr4, 1.5714 - specification and applications

Carburizing steel used on parts requiring high core strength, structures subject to abrasion and variable loads, typically used for small parts such as heavy-duty sprockets, screws, pins, shafts, spigots, machine parts, cars and motors.

 


Mechanical properties - 16NiCrS4, 1.5715 / 16NiCr4, 1.5714

Mechanical properties for individual conditions
Condition Hardness (HBW)
+A <217
+TH 166 - 217
+FP 156 - 207
+S <255

 


Mechanical and physical properties of 17HGN steel

Mechanical and physical properties
Tensile strength Rm ≥ 1030 MPa
Yield point Re ≥ 830 MPa
Hardness in softened condition ≤ 229 HB
Elongation A ≥ 11%
Notch toughness KU2 ≥ 56 J
Contraction Z ≥ 45%
Density ρ 7.85 kg/dm³

Process and temperatures of heat treatment - 16NiCr4, 1.5714, 16NiCrS4, 1.5715

Heat treatment and temperatures
Process time Temperatures
Austenitizing 30 - 35 min 880℃
Carburizing   880 - 980℃
Core-hardening   850 - 890℃
Case-hardening   780 - 820℃
Tempering 1 h minimum 150 - 200℃

 


In the 17HGN grade the company provides:

 


List of equivalents and other determinations of 17HGN steel:

16NiCr4, 1.5714, 16 NiCr 4, 5714, 19ChGN, 19KhGN, 19ХГН, 637H17, 637 H 17, 18ChGN1, 18KhGN1, 18ХГН1, ČSN 16 121, ČSN 16121, 15HGN, 16NiCrS4


We use cookies
In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy. You can specify the detailed configuration by clicking the button below "Settings".
Cookie settings
We use cookies

In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy.

More information

If you have any questions about our cookie policy, please ask contact.