Low-alloy copper construction steel 15NiCuMoNb5-6-4, 1.6368, 15NiCuMoNb5 designed for use at elevated temperatures according to PN-75/H-84024, SEW 028.

 

Standards Steel Grades
Chemical Composition %
C: Mn: Si: P: S: Cr: Mo: Ni: Nb: Ti: Al: Cu: N:
PN 15NCuMNb - K32Nb
<0.17 0.80 - 1.20 0.25 - 0.50 <0.035 <0.035 <0.3 0.25 - 0.40 1.0 - 1.3 0.02 - 0.06 - <0.015 0.5 - 0.8 -
PN 15NCuMNbA - K32NbA
0.13 - 0.17 0.95 - 1.20 0.25 - 0.50 <0.030 <0.030 <0.3 0.25 - 0.40 1.0 - 1.3 0.02 - 0.06 - <0.015 0.5 - 0.8 -
PN 18CuNMT
<0.20 0.70 - 1.00 0.30 - 0.50 <0.040 <0.040 <0.3 0.25 - 0.32 1.0 - 1.2 - 0.03 - 0.05 - 0.9 - 1.2 -
EN
DIN
15NiCuMoNb5-6-4 - 15NiCuMoNb564 - 1.6368 - 6368
<0.17 0.80 - 1.20 0.25 - 0.50 <0.025 <0.010 <0.3 0.25 - 0.50 1.0 - 1.3 0.015 - 0.045 - <0.015 0.5 - 0.8 <0.02
BS BS 591
0.10 - 0.17 0.80 - 1.20 0.25 - 0.50 <0.030 <0.030 <0.3 0.25 - 0.50 1.0 - 1.3 0.045 - 0.050 - <0.045 0.5 - 0.8 <0.02
ISO 9NiMnMoNb5-4-4 - 9NiMnMoNb544
<0.17 0.80 - 1.20 0.25 - 0.50 <0.030 <0.030 <0.3 0.25 - 0.40 1.0 - 1.3 0.015 - 0.045 - <0.020 0.5 - 0.8 -

 

15NiCuMoNb5-6-4, 1.6368 - description and application

Low-alloy steel with copper additive for use at elevated temperatures up to 500 ℃. Products in this steel grade are produced in the form of hot rolled sheets, seamless pipes, hot-rolled and forged bars.

This steel, unlike other grades, has an increased content of nickel and copper. It is used in the construction of boilers for boiler drums, which work up to 375 ℃, high-pressure boilers, pressure vessels, pipelines, nuclear reactors evaporators, chemical apparatus, and other power equipment.

Described copper steel is a former 18CuMNT replacement. In addition, shows great weldability.


Creep limit and creep resistance

Properties (MPa) Temperatures
400℃ 410℃ 420℃ 430℃ 440℃ 450℃ 460℃ 470℃ 480℃ 490℃ 500℃
Rz/10000 402 385 368 348 328 304 274 242 212 179 147
Rz/100000 373 349 325 300 273 245 210 175 139 104 69
R1/10000 324 315 306 295 281 265 239 212 180 145 108
R1/100000 294 279 263 245 227 206 180 151 120 84 49

 


Mechanical properties of 15NiCuMoNb5-6-4, 1.6368 steel

  • For flat products according to EN 10028-2
     
    • The normalized and tempered state +NT
      • Tensile strength Rm = 590 - 780 MPa
      • Yield point Re > 420 MPa
      • Elongation A > 16 %
      • Impact resistance KV20℃ > 40 J/cm2
      • Impact resistance KV0℃nbsp;> 34 J/cm2
      • Impact resistance KV-20℃nbsp;> 27 J/cm2
    • Heat-treated state +QT
      • Tensile strength Rm = 580-740 MPa
      • Yield point Re > 410 MPa
      • Elongation A > 16%
      • Impact resistance KV20℃ > 40 J/cm2
      • impact resistance KV0℃ > 34 J/cm2
      • impact resistance KV-20℃ > 27 J/cm2
  • For seamless tubes according to EN 10216-2
     
    • The normalized and tempered state +NT
      • Tensile strength - Rm > 610 - 780 MPa
      • Yield point Re > 440 MPa
      • Elongation A > 19%
      • impact resistance KV20℃ > 40 J

 


Heat treatment of 15NiCuMoNB5-6-4 steel

  • Normalizationat 880 - 930 °C with cooling in calm air
  • Hardeningat 880 - 930 °C with cooling in oil or water
  • Relief annealingat 580 - 630 °C with cooling in calm air
  • Tempering at a temperature of 600 - 650 °C with cooling in the air

 


In this grade the company provides:

 


Equivalents and other symbols of the 15NCuMNb grade:

15NiCuMoNb5-6-4, 1.6368, 15NiCuMoNb564, 15NiCuMoNb5, 18CuNMT, K32Nb, K32NbA, 15NCuMNbA, BS 591, 9NiMnMoN5-4-4, 9NiMnMoNb544.


We use cookies
In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy. You can specify the detailed configuration by clicking the button below "Settings".
Cookie settings
We use cookies

In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy.

More information

If you have any questions about our cookie policy, please ask contact.