13CrMo4-5, 1.7335, 13CrMo4-4, A182 F11 boiler steel for power engineering in accordance with EN 10273, EN 10222-2, EN 10028-2, and EN 10216-2.

 

Standards Steel Grades
Chemical Composition %
C: Mn: Si: P: S: Cr: Mo: Ni: V: Ti: Cu: W: Al: N:
PN 15HM
0.11 - 0.18 0.4 - 0.7 0.15 - 0.35 <0.04 <0.04 0.7 - 1.0 0.40 - 0.55 <0.35 - - <0.25 - <0.02 -
EN 13CrMo4-5 - 13 CrMo 4-5 - 13CrMo4-4 - 13 CrMo 4-4 - 1.7335
0.08 - 0.18 0.4 - 1.0 <0.35 <0.025 <0.01 0.70 - 1.15 0.4 - 0.6 - - - <0.30 - - <0.012
ISO 14CrMo4-5 - 14 CrMo 4-5
0.10 - 0.18 0.4 - 0.7 <0.40 <0.025 <0.015 0.80 - 1.15 0.4 - 0.6 - - - - - - -
EN 13CrMoSi5-5 - 13 CrMoSi 5-5 - 1.7336
<0.17 0.40 - 0.65 0.50 - 0.80 <0.015 <0.005 1.00 - 1.50 0.45 - 0.65 <0.3 - - <0.3 - - <0.012
AFNOR 15CD4.05 - 15CD4 - 15 CD 4.05
<0.18 0.4 - 0.8 0.15 - 0.35 <0.035 <0.035 0.8 - 1.2 0.4 - 0.6 <0.3 - - - - - -
GOST 15ChM - 15KhM - 15ХМ
0.11 - 0.18 0.40 - 0.70 0.17 - 0.37 <0.035 <0.035 0.80 - 1.10 0.40 - 0.55 <0.3 <0.05 <0.03 <0.3 <0.2 - <0.2
ASTM A182 Grade F11 class 2 and 3 - SA182 F11 class 2 and 3 - UNS K11572
0.1 - 0.2 0.3 - 0.8 0.5 - 1.0 <0.040 <0.040 1.0 - 1.5 0.44 - 0.65 - - - - - - -
ASTM A182 Grade F12 class 1 - SA182 F12 class 1 - UNS K11562
0.05 - 0.15 0.3 - 0.61 <0.5 <0.045 <0.045 0.8 - 1.25 0.44 - 0.65 - - - - - - -
UNS UNS K12062
<0.20 0.3 - 0.8 <0.6 <0.045 <0.045 0.80 - 1.25 0.44 - 0.65 - - - - - - -

 

13CrMo4-5, 1.7335 - Characteristics and application

13CrMo4-5 low alloy steel is a relatively low-carbon chrome-molybdenum grade compared to other related high temperature grades, characterized by good cold and hot workingability, excellent machinability, weldability while maintaining high strength properties at room temperature and elevated temperatures.

The closest equivalent of 13CrMo4-5, more commonly found in the form of products, is used as a half-finished product for parts and subassemblies for the power industry, as well as for chemical industry that work in the temperature up to 530 ℃ - in contact with liquids containing various concentrations of "hard" substances, gases and steam that may contain numerous chemicals - pressure equipment components, boilers, turbines and power systems.

In the 13CrMo4-5 grade are made parts for the fittings for the installations - bottoms, flanges, knee, tees, profiles, seamless tubes, as well as bars, forgings, flat bars and hot rolled sheets with various thickness and dimensions. Earlier mentioned fittings are used for steam and other discharge ducts, such as pipelines and superheater pipes.

For hot rolled, forgings, and forged materials, these products are used for screws, nuts, struts and parts of boilers and steam turbines. Flat products - such as plates or tapes are used as parts for pressure vessels, turbine blades, steamers or steam collectors.

15HM steel is primarily delivered in heat-treated, softened, normalized and tempered state.


Mechanical properties in normalized state for individual dimensions

  • Tensile strength Rm
    • Dimensions: <16 - 60mm = 450 - 600 N/mm2
    • Dimensions: 60 - 100mm = 440 - 590 N/mm2
    • Dimensions: 100 - 150mm = 430 - 580 N/mm2
  • Yield point Rp0.2
    • Dimensions: <16mm = > 300 N/mm2
    • Dimensions: 16 - 60mm = > 295 N/mm2
    • Dimensions: 60 - 100mm = 275 N/mm2
    • Dimensions 100 - 150mm = > 255 N/mm2
  • Notch toughness at room temperature KV
    • Dimensions: 16 - 60mm = > 31 J
    • Dimensions: 60 - 150mm = > 27 J
  • Elongation A
    • Dimensions: 16 - 60mm = > 20 %
    • Dimensions: 60 - 150mm = > 19 %

Heat treatment of 13CrMo4-5 - processes, cooling and temperatures

  • Softening annealing at the temperature of 600 - 700℃
  • Normalizing with cooling in calm air at the temperature of 910 - 940℃
  • Relief annealing with calm air cooling at the temperatures of 660 - 710℃
  • Hardening with cooling in water at the temperature of 890 - 910 ℃, when cooling in oil - 900 - 930 ℃
  • Tempering in calm air at temperatures of 650 - 720 °C

 


Creep limit and creep resistance of 13CrMo4-5 / 1.7335 steel in normalized and tempered state

Properties (MPa) Temperatures
450℃ 460℃ 470℃ 480℃ 490℃ 500℃ 510℃ 520℃ 530℃ 540℃ 550℃ 560℃ 570℃
Rz/10000 363 337 311 284 257 230 201 172 147 125 103 86 73
Rz/100000 284 251 220 190 163 137 116 94 77 61 49 40 33
Rz/200000 260 226 196 167 139 115 96 76 62 47 38 31 25
R1/10000 221 203 186 171 155 141 127 112 98 83 69 54 39
R1/100000 191 172 152 133 116 98 83 70 57 46 36 30 24

 


Virgamet Company in 13CrMo4-5 steel grade provides:

 


Other indications and equivalents of 13CrMo4-5 steel

13CrMo4-5, 13CrMo4.5, 1.7335, 7335, 13CrMo45, 15KhM, 13CrMo4-4, 14CrMo4-5, 13CrMo4.4, 14 CrMo 4-5, 13 CrMo 4-5, 15ChM, 15ХМ, 12ChM, 12KhM, 13CrMoSi5-5, 13 CrMoSi 5-5, 1.7336, 12ХМ, 12CrMo, 15CrMo, 12CrMoG, 15CrMoG, CSN 15121, G17CrMo5-5, 15CD4.05, 15 CD 4.05, BS 620, BS 621, KL 9, Cr5Mo45.47, 12Cr4Mo5H, 15Cr90Mo55, IASC7335, 14CrMo3, SFVA F 12, NV 1 Cr 0.5 Mo, SFVA F12, 14CrMo4, SS 2216, Grade F12, Grade F11, Grade T11, Grade T12, Grade P11, Grade P12, K11562, K11564, K11572, K11597, K12062, K12122, K12822.


We use cookies
In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy. You can specify the detailed configuration by clicking the button below "Settings".
Cookie settings
We use cookies

In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy.

More information

If you have any questions about our cookie policy, please ask contact.