Tool steel for cold- working 100MnCrW4, 1.2510, 95MnWCr5, 1.2825 intended for knives, saws and measuring blades according to ISO 4957.

 

Standard Steel Grade
Chemical Composition %
C: Mn: Si: P: S: Cr: V: W:
PN NMWV
0.9 - 1.0 1.0 - 1.3 0.15 - 0.40 <0.03 <0.03 0.4 - 0.7 0.10 - 0.25 0.4 - 0.7
DIN 100MnCrW4 - 1.2510
0.90 - 1.05 1.0 - 1.2 0.15 - 0.35 <0.035 <0.035 0.5 - 0.7 0.05 - 0.15 0.5 - 0.7
ASTM AISI O1 - UNS T31501
0.85 - 1.00 1.0 - 1.4 0.1 - 0.5 <0.030 <0.030 0.4 - 0.7 <0.3 0.4 - 0.6
ISO 95MnWCr5 - 1.2825
0.9 - 1.0 1.05 - 1.35 0.10 - 0.40 <0.030 <0.030 0.40 - 0.65 0.05 - 0.20 0.4 - 0.7
AF 90MWCV5 - 90MnWCrV5
0.85 - 1.00 1.05 - 1.35 0.10 - 0.40 - - 0.35 - 0.65 0.05 - 0.20 0.4 - 0.7
JIS SKS 3
0.9 - 1.0 0.9 - 1.2 <0.35 <0.030 <0.030 0.5 - 1.0 - 0.5 - 1.0

 

100MnCrW4, 1.2510 - specifications and application

Tool steel for cold-working at low speeds with low tendency to hardening cracking and dimensional deformation while hardening and tempering processes. NMWV and its equivalents are materials exhibiting high hardness, as well as significantly increased resistance to abrasion, what favors cutting processes during operation.

The NMWV and 100MnCrW4/1.2510 grades are used for the production of trimmers and blanking dies, special knives, dies, reamers, cutting saws, broaches, thread and piston rods, taps, milling cutters, broaches, and precision measuring tools. NMWV steel can be used interchangeably with NWC materials.


Mechanical properties of 100MnCrW4, 1.2510:

  • Linear expansion coefficient, α: 11.9 * 10-6 K-1
  • Thermal conductivity, λ: 25 W * m-1 * K-1
  • Hardness in softened condition: <241 HBW
  • Hardness after hardening and tempering:
    • 200℃: >61 HRC
    • 250℃: 60,5 HRC
    • 300℃: 58,8 HRC
    • 350℃: 56,6 HRC
    • 400℃: 54,4 HRC
    • 450℃: 51,8 HRC
    • 500℃: 49,4 HRC
    • 550℃: 46,7 HRC

 


Heat and plastic treatment of 100MnCrW4, 1.2510 steel:

  • Rolling and forging at a temperature of 1050 - 850 ℃
  • Softening annealing at a temperature of 680 - 700 ℃
  • Hardening at a temperature of 780 - 810℃
  • Tempering at a tempering of 150 - 250℃
  • Relief annealing at a temperature of 600 - 650℃

 


In the above mentioned grade, the company provides:

 


Other alternatives and equivalents:

100MnCrW4, 1.2510, 100 MnCrW 4, 95MnWCr5, 1.2825, SKS3, SIS 2140, CSN 19314, BO1, AISI O1, UNS T31501, F-522.A, 90MWCV5, 90 MWCV 5, 90MnWCrV5, 90 MnWCrV 5, 9CrWMn, 9ChVG, 9KhVG, 9ХВГ, 95ХГВФ, 95ChGVF, 95KhGVF.


We use cookies
In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy. You can specify the detailed configuration by clicking the button below "Settings".
Cookie settings
We use cookies

In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy.

More information

If you have any questions about our cookie policy, please ask contact.