X100CrMoV5, 1.2363, AISI A2 - tool steel for cold working according to ISO 4957.

 

Standard Steel Grade
Chemical Composition %
C: Mn: Si: P: S: Cr: Mo: V:
ISO X100CrMoV5-1 - 1.2363
0.95 - 1.05 0.4 - 0.8 0.1 - 0.4 <0.03 <0.03 4.8 - 5.5 0.9 - 1.2 0.15 - 0.35
PN NCLV
0.95 - 1.05 0.4 - 0.7 0.15 - 0.40 <0.03 <0.03 4.5 - 5.5 0.9 - 1.2 0.30 - 0.45
ASTM UNS T30102 - AISI A2
0.95 - 1.05 0.4 - 1.0 0.1 - 0.5 <0.03 <0.03 4.75 - 5.50 0.9 - 1.4 0.15 - 0.50
NF Z100CVD5
0.90 - 1.05 0.5 - 0.8 0.1 - 0.4 - - 4.8 - 5.5 0.9 - 1.3 0.15 - 0.35
JIS SKD12
0.95 - 1.05 0.4 - 0.8 0.1 - 0.4 <0.03 <0.03 4.8 - 5.5 0.9 - 1.2 0.15 - 0.35

 


X100CrMoV5-1, 1.2363, AISI A2 - specifications and applications

Tool steel for cold working with high ductility, high machinability and hardenability, resistant to deformation and cracking during heat treatment. In addition to abrasion resistance, it is a better alternative to tool grades containing 12% of chromium - such as NC10, NC11. It also has better sandability, while keeping its form constant after hardening. This grade is used in the manufacture of tools for metal forming, cold cutting, drawing, stamping and woodworking. 1.2363 / X100CrMoV5-1 is used for the production of large knives, die-cuts, thread rolling jaws, stamping, stamping tools and planing cutters.

 


Mechanical properties of X100CrMoV5-1, 1.2363

  • Hardness in +A condition: <241 HB
  • Hardness in +A +C condition: <261 HB
  • Hardness after hardening: >62 HRC
  • Hardness after hardening and tempering at temperatures:
    • 200℃ = >62 HRC
    • 250℃ = 60.8 HRC
    • 300℃ = 58.0 HRC
    • 350℃ = 57.7 HRC
    • 400℃ = 58.3 HRC
    • 450℃ = 58.4 HRC
    • 500℃ = 56.0 HRC
    • 550℃ = 51.0 HRC
  • Thermal conductivity, λ: 21 W * m-1 * K-1
  • Linear expansion coefficient, α: 10.7 * 10-6 K-1

 


Heat treatment

  • Softening annealing at 800 - 840℃ with furnace cooling
  • Relief annealing at 600 - 700℃
  • Hardening at 940 - 980℃ in oil
  • Tempering at 150 - 550℃ in air
  • Nitriding at 470 - 550℃

 


In the above mentioned grade the company delivers:

 


Other designations of the grade:

SKD 12, X 100 CrMoV 5, X100CrMoV5, 2363, Z100CVD5, Z 100 CDV 5, SS 2260, Cr5Mo1V, A681-94 A2, UNS T30102.


We use cookies
In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy. You can specify the detailed configuration by clicking the button below "Settings".
Cookie settings
We use cookies

In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy.

More information

If you have any questions about our cookie policy, please ask contact.